The Influence of Heat Treatment Processes on Mold Deformation
1. Influence of Heating Rate
In general, a faster heating rate during quenching increases the thermal stress within a mold, making it more prone to deformation or cracking. This is particularly true for alloy steels and high-alloy steels, which have poor thermal conductivity; therefore, preheating is essential. For high-alloy molds with complex geometries, multi-stage preheating may be required. In certain specific cases, however, rapid heating can actually reduce deformation. By heating only the surface of the mold while the core remains "cold," both structural stress and thermal stress are minimized. Furthermore, the core-retaining higher resistance to deformation-helps to limit overall quenching-induced distortion. Practical experience in some manufacturing facilities has shown this approach to be effective in addressing issues related to the deformation of hole spacing.

2. Influence of Heating Temperature
The quenching temperature affects the hardenability of the material, as well as the composition and grain size of the austenite.
(1) Regarding hardenability: A higher heating temperature increases thermal stress. Simultaneously, it enhances hardenability, which in turn increases structural stress-eventually causing the latter to become the dominant factor. For example, with carbon tool steels such as T8, T10, and T12, quenching at standard temperatures typically causes the inner diameter to shrink. However, if the quenching temperature is raised to 850°C or higher, the increased hardenability causes structural stress to become dominant, which may instead lead to an expansion of the inner diameter.

(2) Regarding austenite composition: A higher quenching temperature increases the carbon content within the austenite. This leads to greater tetragonality (and a larger specific volume) of the martensite formed after quenching, resulting in an overall increase in volume.
(3) Regarding the effect on the $M_s$ (martensite start) temperature: Higher quenching temperatures result in coarser austenite grains, which increases the likelihood of the component deforming or cracking. In summary, for all steel grades-especially certain high-carbon, medium-to-high alloy steels-the quenching temperature significantly influences the deformation of molds during the quenching process. Therefore, selecting the appropriate quenching temperature is crucial.

Generally speaking, an excessively high quenching temperature is detrimental in terms of deformation. It is best to use the lowest possible heating temperature, provided that the required service performance is not compromised. However, for steel grades that retain a significant amount of austenite after quenching (such as Cr12MoV), the heating temperature can be adjusted to alter the quantity of retained austenite, thereby controlling the deformation of the mold.

3. Influence of Quenching Cooling Rate
In general, increasing the cooling rate above the $M_s$ (martensite start) temperature significantly raises thermal stresses, which tends to increase deformation caused by these stresses. Conversely, increasing the cooling rate below the $M_s$ temperature primarily tends to increase deformation resulting from microstructural (transformation) stresses.

Because different steel grades have different $M_s$ temperatures, they exhibit varying deformation tendencies even when the same quenching medium is used. Similarly, using different quenching media for the same steel grade-due to their differing cooling capacities-will also lead to different deformation outcomes. For instance, carbon tool steel has a relatively low $M_s$ temperature; when water-quenched, the influence of thermal stress often dominates, whereas oil-quenching may cause microstructural stress to become the dominant factor.

In practical production, when molds undergo staged quenching (martempering) or staged-isothermal quenching, they are typically not quenched completely through the cross-section. Consequently, thermal stress usually plays the primary role, causing the mold cavity to contract; however, since the thermal stress is relatively low in these cases, the total deformation remains minimal. In contrast, if water-oil dual-medium quenching or oil-quenching is employed, the resulting thermal stress is higher, leading to greater contraction of the mold cavity.

4. The Influence of Tempering Temperature
The influence of tempering temperature on deformation is primarily driven by microstructural transformations occurring during the tempering process. If a "secondary hardening" (or "secondary quenching") phenomenon occurs-where retained austenite transforms into martensite-the mold cavity will expand, as the specific volume of the newly formed martensite is greater than that of the retained austenite. For certain high-alloy tool steels (such as Cr12MoV), when high-temperature quenching is employed to achieve "red hardness" (hot hardness) and multiple tempering cycles are performed, the volume increases with each tempering cycle. Conversely, when tempering is conducted within other temperature ranges, the transformation of quenched martensite into tempered martensite (or tempered sorbite, tempered troostite, etc.) results in a decrease in specific volume, causing the mold cavity to contract.

Additionally, the relaxation of residual stresses within the mold during tempering also affects deformation. If the mold surface is under tensile stress following the quenching process, its dimensions will increase upon tempering; conversely, if the surface is under compressive stress, it will undergo contraction. Of these two factors-microstructural transformation and stress relaxation-the former is the primary cause of deformation.